The first step is to press the wax mold
Press the treated wax paste into the mold cavity, take it out after being condensed by the ice water machine, put it into the water tank for a period of time, and obtain a single wax mold after finishing and inspection. Wax mold can be understood as a pressure casting part.
Step 2: manufacturing mould
The mold is used to press the casting pattern. In order to ensure the quality of wax mold, the mold must have high dimensional accuracy and small surface roughness value.
Step 3: mold repair
The quality, surface quality and deformation degree of wax molds determine some important parameters of products. Therefore, the wax mold workshop needs constant temperature control to minimize the deformation of wax molds. At the same time, the surface of each wax mold also needs to be inspected. Those with flow marks should be washed away. At the same time, the burr, flash and clamping line of wax parts should be removed during mold repair, and those with trace defects should be repaired.
Step 4: combine wax molds (Group trees)
After mold repair, for a qualified single wax mold, in order to improve productivity, a single wax mold is fusion welded on the pre prepared wax common gating system to form a wax mold group. Generally, 2 ~ 80 wax molds can be welded on one wax mold group.
Step 5: clean the wax mold
The wax mold group after tree formation can be cleaned after standing for more than 45min. Before shell making and slurry hanging, the wax mold group after the number of groups must be cleaned to remove wax chips and grease on the surface and improve the adhesion of shell making.
Step 6: manufacturing shell
After dipping and hanging the coating outside the wax mold, put it into the shell making room for drying. The surface layer adopts the natural drying method, and the transition layer and back layer adopt the rotary air drying method to accelerate the drying. In this way, the coating and hanging are repeated for 5 ~ 7 times (5 ~ 6 layers for small castings and 6 ~ 9 layers for large castings).
Step 7: shell roasting, pouring, sand falling and cleaning
The dewaxed shell shall be roasted during pouring. The shell shall be roasted in a 1100 ℃ oil fired furnace or electric furnace for 50 minutes. The main purpose is to remove the residual wax after dewaxing, improve the strength and air permeability of the shell and prevent the shell from deformation or rupture during pouring.
Step 8: dewaxing and wax treatment
Pour the mold shell into the steam dewaxing axe to melt the wax mold and flow out from below. Separate it through the water separator, collect the wax liquid, and put it into the water removal bucket to further separate the wax water and remove the impurities in the wax.